RESOURCES/TROUBLESHOOTING

Print Troubleshooting

What’s wrong with your print?

SELECT MATERIAL GRADE
What You May See

Fine, hair-like plastic cobwebs stretching between separate printing structures.

Likely Causes
  • —Nozzle temperature is too high, leading to runny liquid phase polymer.
  • —Retraction distance or speed is set too low for direct or bowden drive extruder.
  • —Filament has absorbed atmospheric moisture.
What to Change
  • 1.Reduce nozzle temperature by 5°C intervals within the recommended range.
  • 2.Adjust retraction parameters (Direct: 0.8–1.5 mm / Bowden: 4.0–6.0 mm).
  • 3.Dry the filament in a dedicated drying chamber before printing.
Polyetra™ PLA Basic Parameter Reference
Recommended Nozzle Temperature: 190–220°CRecommended Bed Temperature: 40–60°C